Brown McFarlane holds stocks of boiler plate steel certified to EN 10028:3 P275NH.
- Ready to be supplied as plate, cut plates, or shapes (profiles).
- The specification EN 10028:3 covers a range of weldable fine grain steels supplied in the normalised condition and intended for pressure purposes.
Requirements
Chemical Requirements
(cast analysis, % by mass, maximum permitted unless indicated otherwise)
C | Si | Mn | P | S | A1 total | N | Cr |
---|---|---|---|---|---|---|---|
0.16 | 0.40 | 0.80-1.50 | 0.025 | 0.015 | 0.020 min | 0.012 | 0.30 |
Cu | Mo | Nb | Ni | Ti | V | Nb+Ti+V | |
0.30 | 0.08 | 0.05 | 0.50 | 0.03 | 0.05 | 0.05 |
Tensile Requirements
Product Thickness | Yield Strength MPa | Tensile Strength MPa | Elongation A% |
---|---|---|---|
up to 16 mm | 275 min | 390 to 510 | 24 min |
16 to 40 mm | 265 min | 390 to 510 | 24 min |
over 40 to 60 mm | 255 min | 390 to 510 | 24 min |
over 60 to 100 mm | 235 min | 370 to 490 | 23 min |
over 100 to 150 mm | 225 min | 360 to 480 | 23 min |
over 150 to 250 mm | 215 min | 350 to 470 | 23 min |
Values
Impact energy values for the normalised condition.
-20°C | 0°C | +20°C | |
---|---|---|---|
Transverse | 30 J min | 40 J min | 50 J min |
Longitudinal | 45 J min | 65 J min | 75 J min |
Strength
Min. values for proof strength Rp0,2 (MPa) at elevated temperatures.
Thickness | 50°C | 100°C | 150°c | 200°C | 250°C | 300°C | 350°C | 400°C |
---|---|---|---|---|---|---|---|---|
up to 16 mm | 266 | 250 | 232 | 213 | 195 | 179 | 166 | 156 |
16 to 40 mm | 256 | 241 | 223 | 205 | 188 | 173 | 160 | 150 |
over 40 to 60 mm | 247 | 232 | 215 | 197 | 181 | 166 | 154 | 145 |
over 60 to 100 mm | 227 | 214 | 198 | 182 | 167 | 153 | 142 | 133 |
over 100 to 150 mm | 218 | 205 | 190 | 174 | 160 | 147 | 136 | 128 |
over 150 to 250 mm | 208 | 196 | 181 | 167 | 153 | 140 | 130 | 122 |